Material | Reference | Material-LC50(30 min + 14 day post)/g m−3 |
---|---|---|
Flexible polyurethane foam | ||
NFR FPU #12 | Levin et al 1983a | 37.8 |
NFR FPU #13 | Levin et al 1986 | 37.0 |
NFR Foam: 22.3 kg m−3 | Braun et al 1990 | 33.0 |
NFR GM-21 | Levin et al 1983b | 27.8 |
NFR GM-21 | Levin et al 1983b | 40.0 |
NFR GM-21 | Levin et al 1983b | 26.6 |
FR FPU #11 | Levin et al 1983a | 17.2 |
FR FPU #14 | Levin et al 1983a | 40.0 |
FR Foam: 22.3 kg m−3 | Braun et al 1990 | 23.0 |
FR GM-23 | Farrar et al 1979 | 12.6 |
FR GM-27 | Farrar et al 1979 | 30.5 |
NFR GM-21 | Farrar et al 1979 | 13.4 |
NFR GM-25 | Farrar et al 1979 | 36.9 |
NFR Foam | Farrar & Galster 1980 | 14.3 |
NFR GM-21: 2 PCF | Anderson et al 1983 | 34.7 |
Rigid polyurethane foam | ||
NFR GM-30 | Levin et al 1983b | 34.0 |
NFR GM-30 | Levin et al 1983b | 39.6 |
NFR GM-30 | Levin et al 1983b | 35.1 |
FR GM-31 | Farrar et al 1979 | 40.0 |
NFR Isocyanurate; GM-41 | Farrar et al 1979 | 8.0 |
NFR isocyanurate; GM-43 | Farrar et al 1979 | 5.0 |
NFR GM-29 | Farrar et al 1979 | 40.0 |
NFR GM-35 | Farrar et al 1979 | 36.7 |
NFR GM-37 | Farrar et al 1979 | 36.7 |
NFR GM-39; sprayed | Farrar et al 1979 | 10.9 |